[melt temperature]: 280-310 ° C
[Cylinder constant temperature]: 220 ° C
[Mold temperature]: 80-110 ° C
[Injection pressure]: Because of the poor fluidity of the material, a high injection pressure is required: 130-180 MPa (1300-1800 bar).
[Pressure pressure]: 40%-60% of the injection pressure; the lower the pressure, the lower the product stress.
[Back pressure]: 10-15MPa (100-150bar)
[Injection speed]: It depends on the flow length and section thickness: thin-walled products require rapid injection; if good surface quality is required, multi-stage slow injection is used.
[screw speed]: The maximum line speed is 0.6 m/s; the plasticizing time corresponds to the cooling time; the screw requires a large torque.
[Measuring stroke]: 0.5-3.5D
[Residual material amount]: 2-6mm, depending on the metering stroke and screw diameter.
[Pre-bake]: Dry at 120 ° C for 3 h; keep the moisture below 0.02%, which will make the mechanical properties better.
[Recovery rate]: Up to 20% of the material can be added; the higher return ratio will maintain heat resistance, but the mechanical properties will be reduced.
[Shrinkage]: 0.6%-0.8%, if it is a glass reinforcement type, 0.2%-0.4%
[Gate system]: The gate diameter should be at least equal to 60%-70% of the wall thickness of the product, but the intersection diameter is at least 1.2mm (the intersection slope is 3-5°, or the surface quality product needs 2°) ); for small products with uniform wall thickness, point gates can be used.
[Barrel equipment]: Standard screw, anti-reverse ring, straight-through nozzle.
[Machine shutdown period]: If the production is interrupted, the machine is operated like an extruder until there is no plastic extrusion and the temperature drops to about 200 °C: clean the barrel, use high-viscosity PE, pull the screw out of the hot barrel and use Wire brush to remove the residue.
[Dongguan Xinxin Plastic Materials Co., Ltd.]
[Plastic knowledge polycarbonate PC engineering plastic engineering plastics PC engineering plastic injection molding knowledge injection molding knowledge]
【Company philosophy】
[Original channels of supply, ensure sufficient stability! Professional technical support, solve problems for you! Accurate market conditions, provide the best price! Standard operating procedures, issued a concept of 17 VAT long-term cooperation. We will be happy to answer your questions about plastics and products. 】
[Contact: Miss Wu] [Contact Phone] [QQ/WeChat]
[Looking forward to your inquiries, or online consultation. 】
Http://news.chinawj.com.cn Plastic knowledge--Polycarbonate PC engineering plastic injection knowledge Editor: (Hardware Business Network Information Center) http://news.chinawj.com.cn Plastic knowledge--Polycarbonate PC engineering plastic injection knowledge

We offer many different standard types of pepper mill mechanism kit, Pepper Grinder Parts kit. All these Pepper Mill Parts kit are conforming to FDA, LFGB requirement. In order to cater to different customers' needs, it includes the metal type grinder pepper mill mechanism, ceramic type grinder Pepper Mill Part Mechanism.

The Pepper Mill Part Kit we supplied are fully adjustable to grind the desired grain size of pepper powder. All of them are very strong, very high efficiency, it can grind all toughest of peppercorns.

The regular length of drive shaft we produced is from 3" to 18" long. Of course, a customized shorter or a longer shaft is available to build. We support a variety of OEM, ODM request.

Pepper Mill Part Kit

Pepper Mill Parts,Pepper Mill Part Mechanism,Pepper Grinder Parts,Pepper Mill Grinder Kit,Pepper Mill Kit For Sale,Pepper Grinder Hardware Kit

Jinghui Industry Ltd. , https://www.ceramictek.com